Wright, Ian ; Bornstein, Norman; Tatlock, Gordon J; Hurley, John
Publication Date:
March 2009
Abstract
The main focus of the work in this Task was the detailed examination and demonstration of
processes for joining tubes made from ODS-FeCrAl alloys. In addition, information on the
high-temperature oxidation behavior in air of ODS-FeCrAl alloys was compiled for use in a
parallel effort to apply thermal barrier coatings to ODS alloys at Cranfield University, in a
UK Task of the overall ODS Alloy Project.
Of the numerous joining techniques for ODS alloys that had been attempted over the years,
two diffusion-based processes were considered to show sufficient promise to warrant further
investigation: transient liquid-phase diffusion (TLP) bonding, and pulsed plasma-assisted
diffusion (PPA) bonding. The main conclusions from this work concerning diffusion-based
joining techniques for producing butt-joints in ODS-FeCrAl tubing are that (1) the PPA
bonding process is capable of producing excellent joints that were demonstrated to exhibit
high retention of axial tensile creep strength at 1000�C in air, with loads to failure up to 82%
of those for monolithic tubes; and (2) the TLP diffusion-bonding process exhibited the
promise shown in earlier investigations that used higher-melting TLP�s but, nevertheless,
suffered from the same drawbacks. The inability to effect the production of a large-grained
microstructure in TLP-bonded joints precluded the development of adequate creep strength.
The causes of this problem were understood, and possible routes to introduce post-TLP
bonding processing steps to promote such recrystallization were considered but not subjected
to any verification testing.
The oxidation behavior in air of ODS-FeCrAl alloys is considered to be well documented for
temperatures in the range 1000 to 1300�C, so that there is an excellent basis for use in
evaluating any improvements resulting from the application of thermal barrier coatings.