Abstract
A crush testing method for hemispherical shell specimens was developed based on the result of finite element (FE) analysis on stress distribution, and was applied to the evaluation of fracture strength for the chemical vapor deposited (CVD) SiC layers of tri-isotropic (TRISO) fuel particles. This report presents descriptions on the testing and evaluation procedures, SiC fracture data, and Weibull statistics parameters.
In the mechanical testing, hemispherical shell specimens of SiC layers removed from TRISO particles were diametrically loaded between a bottom base and a plunger with brass foil at its end. The fracture in the shells always initiates at the inner surface below the loading contact at the convex (outer) surface. Producing a highly uniform stress distribution under the loading contact area is necessary to accurately evaluate the fracture stress from the measured fracture load data by using an analytical solution. Finite element analysis confirms that a relatively soft metal (brass foil) inserted between the specimen�s convex surface and plunger tip produced a highly uniform stress distribution under the contact area.
Nine(9) sets of hemispherical shell specimens were prepared by grinding off 45~50% of the fuel spheres and burning off the carbon layers at 700 �C to obtain free standing SiC. These sample sets were obtained from several relevant lots of coated fuel particles, which include AGR fuels, a German reference fuel, and other development fuels available at Oak Ridge National Laboratory. At least 30 specimens were tested at room temperature for each material and the fracture stress data were analyzed using Weibull statistics. The diameters of the loading-contact area were measured from the impression formed in the brass foil.
The size effect in strength is significant in the specimen size range tested. In this analysis, therefore, the local fracture stress (the fracture stress for the loaded volume only) was calculated from the measurements of fracture load and contact diameter. This was converted to the fracture stress for the full spherical shells, which can be used as reference data for design related analyses. The data listed in the tables are the fracture stress, contact diameters, local fracture stress, fracture stress for the full spherical shell, scale parameter, mean value and Weibull modulus for each data set.
The mean fracture stress varied with test material in the range of 330 � 650 MPa; the values for scale parameter were about 17% higher than the mean fracture stress. Among the test materials B&W-93060 had the lowest fracture stress of about 330 MPa and LEU01-49T exhibited the highest strength at about 650 MPa. The Weibull modulus was in the range of 3.98 � 7.25; the LEU01-46T SiC showed the largest scatter in data and therefore the lowest modulus, 3.98.